Nickel oxide (NiO) is a wide band gap semiconductor material that is used as an electrochromic layer or an ion storage layer in electrochromic devices. In this work, the effect of annealing temperature on sol-gel NiO films was investigated. Fourier transform infrared spectroscopy (FTIR) showed that the formation of NiO via decomposition of the precursor nickel acetate occurred at about 300 °C. Meanwhile, an increase in roughness was observed by Atomic force microscope (AFM), and precipitation of a large number of crystallites was observed at 500 °C. X-ray Diffraction (XRD) showed that the NiO film obtained at such a temperature showed a degree of crystallinity. The film crystallinity and crystallite size also increased with increasing annealing temperature. An ultraviolet spectrophotometer was used to investigate the optical band gap of the colored NiO films, and it was found that the band gap increased from 3.65 eV to 3.74 eV with the increase in annealing temperature. An electrochromic test further showed that optical modulation density and coloring efficiency decreased with the increase in crystallite size. The electrochromic reaction of the nickel oxide film is more likely to occur at the crystal interface and is closely related to the change of the optical band gap. An NiO film with smaller crystallite size is more conducive to ion implantation and the films treated at 300 °C exhibit optimum electrochromic behavior.
The concept of “high entropy” was first proposed while exploring the unknown center of the metal alloy phase diagram, and then expanded to oxides. The colossal dielectric constant found on the bulk high-entropy oxides (HEOs) reveals the potential application of the high-entropy oxides in the dielectric aspects. Despite the fact that known HEO thin films have not been reported in the field of dielectric properties so far, with the high-entropy effects and theoretical guidance of high entropy, it is predictable that they will be discovered. Currently, researchers are verifying that appropriately increasing the oxygen content in the oxide, raising the temperature and raising the pressure during preparation have an obvious influence on thin films’ resistivity, which may be the guidance on obtaining an HEO film large dielectric constant. Finally, it could composite a metal–insulator–metal capacitor, and contribute to sensors and energy storage devices’ development; alternatively, it could be put into application in emerging thin-film transistor technologies, such as those based on amorphous metal oxide semiconductors, semiconducting carbon nanotubes, and organic semiconductors.
In this paper, zirconium–aluminum–oxide (ZAO) dielectric layers were prepared by a solution method with intent to combine the high dielectric constant with a low leakage current density. As a result, dielectric layers with improved electrical properties as expected can be obtained by spin-coating the mixed precursor. The chemical and physical properties of the films were measured by thermogravimetric differential scanning calorimetry (TG-DSC), X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS) and a UV spectrometer. It is observed that the oxygen defects and the hydroxide in the films are reduced with the addition of high-bond-energy zirconia, while the films can remain large optical bond gaps thanks to the presence of alumina. The metal-insulator-metal (MIM) devices were fabricated, and it was seen that with a molar ratio of Zr:Al = 3:1 and an annealing temperature of 500 °C, the dielectric layer afforded the highest dielectric constant of 21.1, as well as a relatively low leakage current of 2.5 10−6 A/cm2@1MV/cm. Furthermore, the indium–gallium–zinc oxide thin-film transistors (IGZO-TFTs) with an optimal ZAO dielectric layer were prepared by the solution method and a mobility of 14.89 cm2/Vs, and a threshold voltage swing of 0.11 V/dec and a 6.1 106 on/off ratio were achieved at an annealing temperature of 500 °C.
Tungsten trioxide (WO3) is a wide band gap semiconductor material, which is commonly not only used, but also investigated as a significant electrochromic layer in electrochromic devices. WO3 films have been prepared by inorganic and sol-gel free ammonium tungstate ((NH4)2WO4), with the modification of glycerol using the spin coating technique. The surface tension, the contact angle and the dynamic viscosity of the precursor solutions demonstrated that the sample solution with a 25% volume fraction of glycerol was optimal, which was equipped to facilitate the growth of WO3 films. The thermal gravimetric and differential scanning calorimetry (TG-DSC) analysis represented that the optimal sample solution transformed into the WO3 range from 220 °C to 300 °C, and the transformation of the phase structure of WO3 was taken above 300 °C. Fourier transform infrared spectroscopy (FT-IR) spectra analysis indicated that the composition within the film was WO3 above the 300 °C annealing temperature, and the component content of WO3 was increased with the increase in the annealing temperature. The X-ray diffraction (XRD) pattern revealed that WO3 films were available for the formation of the cubic and monoclinic crystal structure at 400 °C, and were preferential for growing monoclinic WO3 when annealed at 500 °C. Atomic force microscope (AFM) images showed that WO3 films prepared using ammonium tungstate with modification of the glycerol possessed less rough surface roughness in comparison with the sol-gel-prepared films. An ultraviolet spectrophotometer (UV) demonstrated that the sample solution which had been annealed at 400 °C obtained a high electrochromic modulation ability roughly 40% at 700 nm wavelength, as well as the optical band gap (Eg) of the WO3 films ranged from 3.48 eV to 3.37 eV with the annealing temperature increasing.
Flexible electronic devices have received great attention in the fields of foldable electronic devices, wearable electronic devices, displays, actuators, synaptic bionics and so on. Among them, high-performance flexible memory for information storage and processing is an important part. Due to its simple structure and non-volatile characteristics, flexible resistive random access memory (RRAM) is the most likely flexible memory to achieve full commercialization. At present, the minimum bending radius of flexible RRAM can reach 2 mm and the maximum ON/OFF ratio (storage window) can reach 108. However, there are some defects in reliability and durability. In the bending process, the cracks are the main cause of device failure. The charge trap sites provided by appropriate doping or the use of amorphous nanostructures can make the conductive filaments of flexible RRAM steadier. Flexible electrodes with high conductivity and flexible dielectric with stable storage properties are the main development directions of flexible RRAM materials in the future.
For making full use of the discoloration function of electrochromic (EC) devices and better show the charge and discharge states of supercapacitors (SCs), electrochromic supercapacitors (ECSCs) have attracted much attention and expectations in recent years. The research progress of tungsten-oxide-based electrochromic supercapacitors (ECSCs) in recent years is reviewed in this paper. Nanostructured tungsten oxide is widely used to facilitate ion implantation/extraction and increase the porosity of the electrode. The low-dimensional nanostructured tungsten oxide was compared in four respects: material scale, electrode life, coloring efficiency, and specific capacitance. Due to the mechanics and ductility of nano-tungsten oxide electrodes, they are very suitable for the preparation of flexible ECSCs. With the application of an organic protective layer and metal nanowire conductive electrode, the device has higher coloring efficiency and a lower activation voltage. Finally, this paper indicates that in the future, WO3-based ECSCs will develop in the direction of self-supporting power supply to meet the needs of use.