Currently, silicon and silicon-based composite materials are widely used in microelectronics and solar energy devices. At the same time, silicon in the form of nanoscale fibers and various particles morphology is required for lithium-ion batteries with increased capacity. In this work, we studied the electrolytic production of nanosized silicon from low-fluoride KCl–K2SiF6 and KCl–K2SiF6–SiO2 melts. The effect of SiO2 addition on the morphology and composition of electrolytic silicon deposits was studied under the conditions of potentiostatic electrolysis (cathode overvoltage of 0.1, 0.15, and 0.25 V vs. the potential of a quasi-reference electrode). The obtained silicon deposits were separated from the electrolyte residues, analyzed by scanning electron microscopy and spectral analysis, and then used to fabricate a composite Si/C anode for a lithium-ion battery. The energy characteristics of the manufactured anode half-cells were measured by the galvanostatic cycling method. Cycling revealed better capacity retention and higher coulombic efficiency of the Si/C composite based on silicon synthesized from KCl–K2SiF6–SiO2 melt. After 15 cycles at 200 mA·g−1, material obtained at 0.15 V overvoltage demonstrates capacity of 850 mAh·g−1.
Nowadays, research aimed at the development of materials with increased energy density for lithium-ion batteries are carried out all over the world. Composite anode materials based on Si and C ultrafine particles are considered promising due to their high capacity. In this work, a new approach for carbothermal synthesis of C/SiC composite mixtures with SiC particles of fibrous morphology with a fiber diameter of 0.1–2.0 μm is proposed. The synthesis was carried out on natural raw materials (quartz and graphite) without the use of complex equipment and an argon atmosphere. Using the proposed method, C/SiC mixture as well as pure SiC were synthesized and used to manufacture anode half-cells of lithium-ion batteries. The potential use of the resulting mixtures as anode material for lithium-ion battery was shown. Energy characteristics of the mixtures were determined. After 100 cycles, pure SiC reached a discharge capacity of 180 and 138 mAh g−1 at a current of C/20 and C, respectively, and for the mixtures of (wt%) 29.5C–70.5 SiC and 50Si–14.5C–35.5SiC discharge capacity of 328 and 400 mAh g−1 at a current of C/2 were achieved. The Coulombic efficiency of the samples during cycling was over 99%.
1
1 February 2022 in Journal of the Electrochemical Society
In this paper we report characteristics and electrochemical properties of silicon fibers used as lithium-ion battery anode. All samples were synthesized by potentiostatic electrodeposition from molten KCl–K2SiF6. From molten KCl–CsCl–K2SiF6 deposition was carried out in galvanostatic mode. Despite the synthesis in inert atmosphere and absence of oxygen containing compounds in the melt resulting silicon after washing contains at least 15 at% oxygen. Silicon fibers synthesized at −250 mV (vs Si) were the thinnest with diameter as small as 100 nm; average fiber length increased with increasing overvoltage. Addition of CsCl to the melt results in decrease of the average fibers diameter. Silicon fibers synthesized at −250 mV (vs Si) in KCl–K2SiF6 melt showed the best cycling performance with capacity of 1030 mAh·g−1 at 0.2 A·g−1 discharge current and capacity of 715 mAh·g−1 after 10 cycles. Lithium diffusion coefficients calculated from galvanostatic intermittent titration technique (GITT) are common for silicon-based anode. The highest initial diffusion coefficient value of 6.68·10−11 cm2·s−1 was achieved for silicon synthesized from melt with addition of CsCl. Low capacity and rapid capacity fading for all samples can be caused by high silicon dioxide content, further treatment of synthesized silicon is necessary to achieve higher performance.
Silicon and silicon-based materials are increasingly used in microelectronics, metallurgy and power generation. To date the active study aimed at the development of silicon materials to be used in devices for solar energy conversion, accumulation and storage is underway. In addition, silicon is a promising anode material for lithium-ion fuel cells. In the present paper a possibility of silicon electroreduction from the NaI–KI–K2SiF6 melt in the argon atmosphere is studied. With this aim in view the electrolysis of the NaI–KI–K2SiF6 melt with glassy carbon cathode was performed under galvanostatic and potentiostatic regimes at the temperatures ranging from 650 to 750 °С. The morphology, phase and elemental analyses of the obtained silicon deposits were performed after their separation from the electrolytes by the ICP, SEM-EDX, XRD and Raman spectroscopy methods. Fiber and thread-like silicon samples of 60 to 320 nm in dimeter with admixtures concentrations (mainly oxygen) from 1.2 to 4.6 wt.% were experimentally synthesized. The obtained samples were tested as possible Si/C composite anodes for lithium-ion power sources. The discharge capacity of such power sources after 30 cycles of lithiation-delithiation ranged from 440 to 565 mAh·g–1 and the coloumbic efficiency ranged from 89 to 91%.
1
1 December 2021 in Journal of the Electrochemical Society
Texturing silicon wafers is one way to increase the performance of solar cells. This work is the first to report on the surface modification of Si wafers by processing in polytungstate melts. Scanning electron microscopy (SEM), atomic force microscopy (AFM), X-ray diffraction analysis (XRD), the Brunauer–Emmett–Teller (BET) method, and photoelectrochemical measurements were used to elucidate the effect of texturing conditions in the Na 2 WO 4 —K 2 WO 4 (1:1) melt containing 35 or 50 mol% WO 3 at 973 K in air. As a result of cathodic treatment in the melt containing 50 mol% WO 3 at the potential of –0.92 V (vs Pt) for 15 s, upright pyramids were formed on the Si surface. In addition, inverted pyramids appeared at the OTB/Si contact points. The photocurrent density of these samples was several times higher than that for the initial Si wafer or the Si wafer etched in 5 M NaOH solution at 353 K for 20 min. Mechanisms for the formation of upright and inverted pyramids were proposed. Unusual eight-faceted pyramids were formed on the Si surface during cathodic treatment in the melt containing 35 mol% WO 3 at –1.19 V for 15 s, but the photocurrent density of such samples was low.
Silicon is one of the promising anode materials for lithium-ion batteries with enhanced performance. However, the degradation of silicon during lithiation/delithiation is still the main problem that prevents it commercial use as electrodes. In this work the behavior of a silicon film of about 5–6 µm thick electrodeposited from LiCl-KCl-CsCl-K2SiF6 melt on glassy carbon was studied during its lithiation and delithiation, the film being a part of the anode half-cell of a lithium-ion battery. For this purpose, the methods of cycling in galvanostatic mode, electrochemical impedance, and scanning electron microscopy were used. The principal possibility of lithiation/delithiation of the film was shown and its energy characteristics during multiple cycling were determined. However, during 714 charge-discharge cycles with the current being 0.84 A/g the discharge capacity decreased from 723 to 58 mA·h/g. It was noted that the cause of degradation of the investigated sample was the detachment of the film from the glassy carbon substrate and its cracking.