New experimental results have been obtained on the behavior of arsenic and other associated metals (Re and others) under conditions of oxidative and reductive sintering. It has been established that the extraction of arsenic strongly depends on the process temperature during oxidative sintering. The extraction of arsenic into dust media at 873 K is 50% and rhenium is 88–90%. The effect of excess air on the extraction of arsenic and rhenium into dust was studied: the higher the excess air coefficient, the more complete the extraction of arsenic and rhenium into the dust. The obtained data indicate that achieving a high level of arsenic extraction from the initial product is not possible during oxidative sintering. The best arsenic removal results were reached under the conditions of reductive sintering of initial material by natural gas. The extraction of arsenic into dust at 823 K was 88%, and at 1373 K arsenic is almost completely converted into dust. Obtained new experimental results have a fundamental importance for the selection and organization of a comprehensive technology for the processing complex in composition refractory gold-copper-arsenic-bearing products.
Fine dust from copper smelting plants is an important source of raw materials for the extraction of various valuable metals. A specific feature of dust from copper smelting plants in Kazakhstan is their high arsenic content of up to 15%. This work shows the possibility of hydrometallurgical processing of fine dust from copper smelters, obtained during the converting of copper mattes through the Vanyukov process, via direct leaching with sulfuric acid. The influence of temperature, process time and the S:L (solid/liquid) ratio on the selective extraction of Pb, Zn, Cu and As into targeted products under leaching conditions is studied. The results of the test work show that with the optimal process parameters of S:L = 1.5, t = 60 °C, τ = 60 min, the extraction of copper and zinc into solution is achieved as 89% and 96%, respectively, and lead into cake by up to 97%. The relatively low extraction of copper and zinc into the solution is explained by the transition of copper and zinc ferrites that are insoluble in sulfuric acid into the lead cake. The redistribution of arsenic between the leaching products established in this case also affects the reduction in copper and zinc in the solution. The extraction of arsenic into the solution is 49.32%. More than half of the arsenic from the dust is left in the lead cake. The concentration of arsenic in lead cake will lead to its transition into circulating dust during smelting. This will increase the accumulation of arsenic in the overall process flow. Therefore, when organizing dust-processing technology, it is necessary to provide measures for the preliminary removal of arsenic.
The issues of smelting of difficult for treatment high-sulfur copper-zinc concentrate together with semiproducts and reverts of lead manufacture are considered. The possibility of direct extraction of copper, lead and zinc from copperzinc concentrate to target products in a one-stage process is substantiated. Presented are the results of laboratory meltings for coprocessing of lead semiproducts, reverts and copper-zinc concentrate at a temperature of 1250 °С under the melt bubbling conditions. High indexes of metal extraction into target products were achieved: copper into matte – up to 95% against 88.9% according to the existing technology; lead into lead bullion – up to 94% against 70.8% and zinc into slag – up to 95% compared to 83.7%. Extraction of arsenic and antimony into dust – 91 and 92.3% compared to 69.5% and 59.8%, respectively, which provides circumstances for their removal from the overall process chain of lead production. The use of the proposed solution in lead production will lessen the load on the environment; improve the process figures of the blast concentrating smelting process by reducing the loss of copper, lead with slag and high recovery of arsenic and antimony into dust. Compared to the existing technology, the consumption of coke and quartz flux is significantly reduced: from 6.7 to 2.5% and from 12.5 to 4.7% of the charge weight, respectively. The results of comelting of lead semiproducts and copper-zinc concentrate can form the basis for the development of a new manufacturing method.