The design of zirconia-based scaffolds using conventional techniques for bone-regeneration applications has been studied extensively. Similar to dental applications, the use of three-dimensional (3D) zirconia-based ceramics for bone tissue engineering (BTE) has recently attracted considerable attention because of their high mechanical strength and biocompatibility. However, techniques to fabricate zirconia-based scaffolds for bone regeneration are in a stage of infancy. Hence, the biological activities of zirconia-based ceramics for bone-regeneration applications have not been fully investigated, in contrast to the well-established calcium phosphate-based ceramics for bone-regeneration applications. This paper outlines recent research developments and challenges concerning numerous three-dimensional (3D) zirconia-based scaffolds and reviews the associated fundamental fabrication techniques, key 3D fabrication developments and practical encounters to identify the optimal 3D fabrication technique for obtaining 3D zirconia-based scaffolds suitable for real-world applications. This review mainly summarized the articles that focused on in vitro and in vivo studies along with the fundamental mechanical characterizations on the 3D zirconia-based scaffolds.
This study compared the surface roughness, contact angle, surface energy, residual monomers, degree of conversion, and flexural strength of 3D-printed dental resin under various washing conditions. The specimens were printed with a digital light processing (DLP) printer and were divided into four groups: the group dipped in IPA for 5 s (IPA-D), the group washed in IPA for 1 min (IPA-1), the group washed in IPA for 10 min (IPA-10), and the group washed with TPM for 10 min (TPM-10). Following, the groups were redivided into two groups: a cured group and an uncured group. All experimental data were statistically analyzed using one-way analysis of variance and Tukey’s test. In all groups, the surface roughness showed a value of 1.2–1.8 μm, with no significant difference (p > 0.05). Contact angle showed a significant difference between the three groups using IPA and the TPM group, whereby the TPM-washed specimen showed a low contact angle (p < 0.05). The degree of conversion (DOC) increased in the following order: IPA-D group, IPA-1 group, IPA-10 group, and TPM-10 group, exhibiting a significant difference between all groups (p < 0.05). Flexural strength was measured at 110–130 MPa in all groups, with no significant difference between groups (p > 0.05). The washing time and washing solution type of the 3D printing material had no significant effect on surface roughness and flexural strength.
In this study, we have analysed the effects of a silane coupling agent on the volume fraction of zirconia for digital light processing (DLP)-based additive manufacturing processes. Zirconia suspension was prepared by the incorporation of silane-modified zirconia particles (experimental group) or untreated zirconia particles (control group). Furthermore, the control and experimental group were subdivided into three groups based on the volume fraction (52, 54, and 56 vol%) of zirconia particles. The disk-shaped zirconia samples were 3D (three-dimensional) printed using the DLP technique and their physical and mechanical properties were evaluated. The addition of a silane coupling agent to the zirconia samples was found to have influence of about 6% on the hardness and biaxial flexural strength. Moreover, the decrease in minute air gaps inside the zirconia layers significantly increased the material density (visualized from the microstructure analysis). Thus, from this study, it was established that the silane-modified zirconia particles had a positive effect on the physical properties of the zirconia parts.
We evaluated the effect of electron beam (E-beam) sterilization (25 kGy, ISO 11137) on the degradation of β-tricalcium phosphate/polycaprolactone (β-TCP/PCL) composite filaments of various ratios (0:100, 20:80, 40:60, and 60:40 TCP:PCL by mass) in a rat subcutaneous model for 24 weeks. Volumes of the samples before implantation and after explantation were measured using micro-computed tomography (micro-CT). The filament volume changes before sacrifice were also measured using a live micro-CT. In our micro-CT analyses, there was no significant difference in volume change between the E-beam treated groups and non-E-beam treated groups of the same β-TCP to PCL ratios, except for the 0% β-TCP group. However, the average volume reduction differences between the E-beam and non-E-beam groups in the same-ratio samples were 0.76% (0% TCP), 3.30% (20% TCP), 4.65% (40% TCP), and 3.67% (60% TCP). The E-beam samples generally had more volume reduction in all experimental groups. Therefore, E-beam treatment may accelerate degradation. In our live micro-CT analyses, most volume reduction arose in the first four weeks after implantation and slowed between 4 and 20 weeks in all groups. E-beam groups showed greater volume reduction at every time point, which is consistent with the results by micro-CT analysis. Histology results suggest the biocompatibility of TCP/PCL composite filaments.
Stereolithography (SL) can fabricate complex ceramic parts layer by layer using computer-aided design (CAD) models. The traditional SL system utilizes a vat filled with ceramic slurry with a high solid content, which for ceramics contributes to several limitations and operational difficulties, and further renders it nonrecyclable mainly due to the presence of printed residue and its high viscosity. In this study, we utilized a continuous film supply (CFS) system integrated with a tape-casting type digital light processing (DLP) printer to fabricate zirconia prototypes with a solid content of 45 volume percent (vol.%). Various printing and postprocessing parameters were studied for optimization, to achieve a relative density of 99.02% ± 0.08% with a microhardness of 12.59 ± 0.47 GPa. Slurry reusability was also demonstrated by printing with recycled slurry to produce consistent relative density values in the range of 98.86% ± 0.02% to 98.94% ± 0.03%. This method provides new opportunities for material recycling and the fabrication of dense complex ceramic products, reducing the consumption of the material.
This study evaluated the effect of UV absorbers on the dimensional accuracy of zirconia specimens fabricated by additive manufacturing using a digital light process. Zirconia suspension for additive manufacturing was prepared by setting the volume fractions (0, 0.005, 0.05, and 0.1%) of various UV absorbers. The effect of UV absorber content was evaluated through curing thickness, geometric overgrowth model design, linear deviation, and microstructure evaluation before and after sintering. Statistical analysis was performed by Kruskal–Wallis H and post-tested by the Bonferroni correction method. There was no significant difference in the cure depth according to the presence or absence of the UV absorber, the difference in geometric overgrowth was from 2.1 to 12.5%, and the overgrowth significantly decreased as the amount of added UV absorber increased. This result may contribute to improved precision of 3D multilayer ceramic products.