Immiscible Cu-Fe alloys exhibit poor corrosion resistance due to different corrosion potentials between the constituent phases, which limits their application. In this paper, a composite gradient-structured Cu-10 wt.%Fe plate was prepared via the ultrasonic surface rolling process (USRP). The microstructure evolution, mechanical properties and corrosion behavior were studied. The results demonstrate that USRP effectively enhances both the strength and corrosion resistance of the Cu-10Fe alloy. The improved strength is related to the combined effects of Hall–Petch strengthening, dislocation strengthening, and additional strengthening resulting from homogeneous deformation between the surface layer and the matrix. The enhanced corrosion resistance is primarily attributed to the refined microstructure of the surface layer after USRP, which facilitates the formation of a protective passivation film.
This study investigates the impact of strain rate on the twinning process (i.e., twin nucleation, twin propagation, and twin growth) and associated mechanical behavior during compression along the normal direction (ND) and transverse direction (TD) of a rolled AZ31 Mg plate at a range of strain rates from 0.00005 s−1 to 2500 s−1. The findings reveal that the yield strength is insensitive to strain rates below 0.05 s−1 during both ND and TD compression tests, while at higher strain rates of 2500 s−1, the yield strength increases under both loading conditions. Interestingly, the TD-compressed sample exhibits a larger yield plateau at a strain rate of 2500 s−1, attributed to an increased activation of {102} twins. Further examination of the microstructure reveals that the twinning process is highly dependent on the strain rate. As the strain rate increases, twin nucleation is promoted, leading to a higher twin boundary density. In contrast, at lower strain rates, twin nucleation is restrained, and the external strain is mainly accommodated by twin growth, which results in higher area fractions of twinned regions.
Cu-Ni-Si is a prominent example of a high-end lead frame copper alloy. The enhancement of strength without compromising electrical conductivity has emerged as a prominent research focus. The evolution of the precipitates exerts a significant influence on the strength and electrical conductivity of Cu-Ni-Si-Co-Mg alloys. In this paper, the effects of aging treatment and Mg addition on the properties and precipitates of cold-rolled Cu-Ni-Si-Co alloys were studied. The precipitate was (Ni, Co)2Si and was in a strip shape. During aging, precipitation and coarsening of the (Ni, Co)2Si precipitates were observed. In the early stage of aging, a significant number of fine (Ni, Co)2Si precipitates were formed. These fine precipitates could not only have a better effect of precipitation strengthening, but also impeded the dislocation movement, thus increasing the dislocation density and improving the dislocation strengthening effect. However, the coarsening of the precipitates became dominant with increasing aging times. Therefore, the strengthening effect was weakened. The addition of 0.12% Mg promoted finer and more diffuse precipitates, which not only improving the tensile strength by 100–200 MPa, but also exhibiting a smaller effect on the electrical conductivity. However, further increases in Mg contents resulted in a significant decrease in electrical conductivity, with little change in the tensile strength. The optimum amount of added Mg was 0.12%, and the aging parameters were 300 °C and 20 min.
Magnesium (Mg) alloy sheets usually suffer from severe mechanical anisotropy and a trade-off between strength and ductility. In this work, the effects of rolling temperature (200 °C and 400 °C) and rolling speed (50–1000 r/min) on the microstructure and mechanical properties of a Mg-1Sm (samarium, Sm) (wt.%) alloy were systematically investigated. Low-temperature rolling (200 °C) results in high dislocation density and a double-peak basal texture in Mg-1Sm alloy, causing very limited plasticity and a pronounced anisotropy with a lower yield strength along the rolling direction (RD) than along the transverse direction (TD). A significantly improved mechanical property (yield strength of ~196 MPa, elongation of 18.4% and near-isotropy) can be achieved in the Mg-1Sm alloy by optimizing the rolling conditions (400 °C, 500 r/min). The findings indicate that increasing the temperature is beneficial for activating non-basal slip and multiple twinning modes, thereby weakening and dispersing the basal texture, which can efficiently improve the anisotropic properties. Increasing the rolling speed can promote the recrystallization process, resulting in the enhancement of plasticity. Quantitative analyses reveal that the reduction in dislocation density and the suppression of Sm segregation at grain boundaries under high-temperature high-speed rolling are responsible for the improved ductility and reduced anisotropy.
Understanding the distinct roles of representative alloying elements, including rare-earth (RE) solutes such as Gd and Y and non-rare-earth (non-RE) solutes such as Al and Zn, in regulating microstructural evolution and mechanical response is essential for developing high-strength Mg sheets. In this study, Gd and Y are typical RE solutes, whereas Al and Zn are common non-RE alloying elements, and were individually added to pure Mg at an identical concentration of 0.3 at.% to enable a controlled comparison of their effects on microstructural evolution and mechanical response during hot rolling and subsequent annealing. The effects of alloying elements on hot-rolling behavior were first investigated. Mg-Al and Mg-Zn exhibited improved hot rollability, whereas Mg-Gd and Mg-Y showed higher edge-cracking susceptibility after 90% hot rolling. The hot-rolled (HR) Mg-Gd and Mg-Y sheets achieved yield strength (YS) values of 235.5 and 226.4 MPa, respectively, exceeding those of Mg-Al (170.0 MPa) and Mg-Zn (162.8 MPa). Combined microstructural characterizations and DFT calculations revealed that RE solutes strongly segregated at grain boundaries, inducing solute drag, suppressing dynamic recrystallization (DRX), and promoting dislocation accumulation. During subsequent annealing, the grain size increased by only ~1.5 times in Mg-Gd/Mg-Y, whereas increases of 2.6–2.96 times were observed in pure Mg and Mg-Al/Mg-Zn alloys. The RE-containing alloys retained a UTS of ~190 MPa and elongations above 12% after annealing at 500 °C for 240 min. The identical atomic fraction design (0.3 at.%) enabled a direct comparison of the element-specific effects of different alloying elements, providing insights into alloy design and thermomechanical processing strategies for high-performance Mg sheets.