This study investigates the effect of hydrogen embrittlement on the fracture toughness of 9% Ni steel and STS 316L stainless steel under cryogenic conditions ranging from −80 °C to −253 °C. Hydrogen charging was performed using electrochemical methods, and hydrogen uptake was quantitatively analyzed using thermal desorption spectroscopy (TDS). Fracture toughness was evaluated using crack tip opening displacement (CTOD) testing per ISO 12135, both without hydrogen (WO-H) and with hydrogen (W-H). The results showed a gradual decrease in CTOD values with decreasing temperature in both steels under hydrogen-free conditions, with ductile fracture maintained even at −253 °C. In contrast, hydrogen-charged specimens exhibited significant toughness degradation at intermediate subzero temperatures (−80 °C to −130 °C), particularly in 9% Ni steel due to its BCC crystal structure. However, at −160 °C and below, the effect of hydrogen embrittlement was suppressed mainly owing to the reduced hydrogen diffusivity. Scanning electron microscopy (SEM) analysis confirmed the transition from ductile to brittle fracture with decreasing temperature and hydrogen influences. At −253 °C, fully brittle fracture surfaces were observed in all specimens, confirming that at ultra-low temperatures, fracture behavior is dominated by temperature effects rather than hydrogen. These findings identify a practical temperature limit (approximately −160 °C) below which hydrogen embrittlement becomes negligible, providing critical insights for the design and application of structural materials in hydrogen cryogenic environments.
This study examines the residual stress characteristics of spot welding in newly developed high-strength steel for automotive body construction through experimental and numerical methods. The effects of sheet thickness, nugget size, and the presence or absence of spacers on residual stress distribution and fracture stability were evaluated. Measurements using XRD and HDR revealed tensile residual stress below the yield strength at the nugget center. A numerical analysis system corroborated experimental findings, demonstrating that larger nugget sizes reduce tensile residual stress at the nugget center, enhancing fracture stability. However, for nugget sizes of 3 (t: thickness), high tensile stress at the nugget edge compromised stability, while sizes of 3.5 or larger improved fracture resistance. The study also found that thicker sheets increased fracture safety with larger nugget sizes, and the presence of spacers induced tensile stress through spring-back effects, which shifted to compressive stress as the nugget size increased. These results provide critical insights into optimizing welding parameters to improve the structural integrity of automotive components.
In this study, fracture toughness with the base metal of 9% Ni steel, a cryogenic steel, was evaluated under conditions without hydrogen charging (WO-H) and with hydrogen charging (W-H). Hydrogen charging was performed using an electrochemical cathodic charging method in a electrolyte of 3% NaCl + 0.3% NH4SCN at 19℃ with a current density of 50 A/m². Fracture toughness was assessed at -80℃, -100℃, -130℃, and -160℃ using CTOD (Crack Tip Opening Displacement) tests. The results for WO-H indicated a decrease in fracture toughness values with decreasing temperature, while the results for W-H showed an increase in fracture toughness values as the temperature decreased. In addition, the fracture surfaces and fracture toughness of WO-H and W-H became increasingly similar as the temperature decreased, as observed through scanning electron microscopy (SEM). At -80℃, there was a significant difference in fracture toughness between the WO-H and W-H conditions. WO-H was influenced only by the low temperature, whereas W-H was affected by both low temperature and hydrogen, showing combined effects that led to a decrease in fracture toughness due to hydrogen embrittlement. However, at -160℃, the fracture toughness values for both WO-H and W-H conditions were nearly identical. This suggests that the temperature effect on fracture toughness reduction is greater than hydrogen embrittlement at very low temperatures.
In this study, a novel estimating equation based on the WES2808 standard was proposed to predict fracture toughness through the transition temperature of Charpy impact toughness and CTOD (Crack Tip Opening Displacement) fracture toughness. This equation was specifically developed for 460MPa class H-section steel materials used in marine structures, including the base material (BM), heat-affected zone (HAZ), and weld metal (WM). The experimental results confirmed that the proposed estimation equation accurately predicted the fracture toughness across these different material regions. These findings demonstrate the reliability and applicability of the proposed equation in estimated fracture toughness for marine structure materials, thereby contributing to improved safety and performance in harsh environmental conditions.