High-manganese austenitic steel was developed to improve the fracture toughness and safety of steel under cryogenic temperatures, and its austenite structure was formed by increasing the Mn content. The developed high-manganese austenitic steel was alloyed with austenite-stabilizing elements (e.g., C, Mn, and Ni) to increase cryogenic toughness. It was demonstrated that 30 mm thickness high-manganese austenitic steel, as well as joints welded with this steel, had a sufficiently higher fracture toughness than the required toughness values evaluated under the postulated stress conditions. High-manganese austenitic steel can be applied to large offshore and onshore LNG storage and fuel tanks located in areas experiencing cryogenic conditions. Generally, fracture toughness decreases at lower temperatures; therefore, cryogenic steel requires high fracture toughness to prevent unstable fractures. Brittle fracture initiation and arrest tests were performed using 30 mm thickness high-manganese austenitic steel and SAW joints. The ductile fracture resistance of the weld joints (weld metal, fusion line, fusion line + 2 mm) was investigated using the R-curve because a crack in the weld joint tends to deviate into the weld metal in the case of undermatched joints. The developed high-manganese austenitic steel showed little possibility of brittle fracture and a remarkably unstable ductile fracture toughness.
This study investigates the effect of hydrogen embrittlement on the fracture toughness of 9% Ni steel and STS 316L stainless steel under cryogenic conditions ranging from −80 °C to −253 °C. Hydrogen charging was performed using electrochemical methods, and hydrogen uptake was quantitatively analyzed using thermal desorption spectroscopy (TDS). Fracture toughness was evaluated using crack tip opening displacement (CTOD) testing per ISO 12135, both without hydrogen (WO-H) and with hydrogen (W-H). The results showed a gradual decrease in CTOD values with decreasing temperature in both steels under hydrogen-free conditions, with ductile fracture maintained even at −253 °C. In contrast, hydrogen-charged specimens exhibited significant toughness degradation at intermediate subzero temperatures (−80 °C to −130 °C), particularly in 9% Ni steel due to its BCC crystal structure. However, at −160 °C and below, the effect of hydrogen embrittlement was suppressed mainly owing to the reduced hydrogen diffusivity. Scanning electron microscopy (SEM) analysis confirmed the transition from ductile to brittle fracture with decreasing temperature and hydrogen influences. At −253 °C, fully brittle fracture surfaces were observed in all specimens, confirming that at ultra-low temperatures, fracture behavior is dominated by temperature effects rather than hydrogen. These findings identify a practical temperature limit (approximately −160 °C) below which hydrogen embrittlement becomes negligible, providing critical insights for the design and application of structural materials in hydrogen cryogenic environments.
When evaluating the safety of steel structures, welding residual stress is used as the secondary load and if there is any restraint, the yield stress of the base material is used for secondary load, regardless of the size of the restraint. Of late, as the yield stress of members is increasing with the increase in the use of high-strength steels, the proportion of the residual welding stress in the total load during the evaluation of the safety of structures is increasing. Therefore, it is necessary to investigate the effect of the size of the restraint on the residual welding stress, determine reasonable residual stress according to the size of the restraint, and apply the residual stress as a secondary load. To investigate the effect of constraint conditions on residual welding stress, thermoelastic–plastic analysis was performed for different member thicknesses, yield stresses, and constraint sizes. The restraint did not affect the residual stress in the direction of the weld line but did affect the residual stress in the direction perpendicular to the weld line. The restraint moved the tensile stress to the compression stress in the direction perpendicular to the weld line at the first layer of the weld and moved the compression stress to the tensile stress at the middle and final layers of the weld. The change in residual stress was the largest in the middle of the weld.
Using high-strength steel for offshore structures with a yield stress of 500 MPa, this study evaluated the distribution characteristics of welding residual stress in the thickness direction under the influence of constrained conditions during welding using cutting, neutron diffraction, and contour methods. Welding residual stress inevitably occurs during welding and impacts fracture stability in structures. As high-strength steel better reflects the effects of phase transformation, the behavior of welding residual stress is known to differ from that of general steel. This study fabricated fully constrained and unconstrained specimens and evaluated them under identical conditions to evaluate welding residual stress according to the influence of constraints on high-strength steel welds. The results indicated that the maximum tensile residual stress of the fully constrained specimen occurred in the first layer of the weld joint, while the maximum tensile residual stress of the fully unconstrained specimen occurred in the last layer of the weld joint. Additionally, the welding residual stress of the fully constrained specimen was larger. Although some errors occurred in the residual stress values in the thickness direction depending on the measurement method, both methods applied in this study exhibited nearly identical distributions. Meanwhile, a maximum angular deformation of about 6° occurred in the fully unconstrained specimen, and we considered that the residual stress decreased owing to the occurrence of angular deformation. The maximum welding residual stress is generally the degree of yield stress. When residual stress greater than the yield stress occurs, it changes to the plastic range and appears in the form of angular, longitudinal, and lateral deformation. Under the fully unconstrained condition, reduced residual stress is considered to appear in the form of angular deformation. The welding tensile residual stress decreased to around 42% in the unconstrained specimen compared to the constrained specimen, and at that time, angular deformation of approximately 6° occurred. Therefore, it is estimated that an angular distortion of about 2.4° occurs as the stress of 100 MPa decreases.
Unstable fractures tend to occur after ductile crack initiation or propagation. In most collapsed steel structures, a maximum 15% pre-strain was recorded, at the steel structural connections, during the great earthquake of 1995, in Japan. Almost-unstable fractures were observed in the beam-to-column connections, where geometrical discontinuities existed. Structural collapse and unstable failure occurred after large-scale plastic deformations. Ship structures can also suffer from unstable fractures in the welded joints. The fracture resistance of butt-welded joints subjected to tension in the pre-strained condition was estimated by considering the toughness deterioration, due to pre-strain and toughness correction for constraint loss in a tension specimen. The target specimen for this fracture assessment was a double-edged, through-thickness crack panel, with a crack in the weld joint (heat-affected zone (HAZ)). The critical fracture toughness value (crack tip opening displacement (CTOD)) of a large structure with pre-strain, which was applied to the HAZ region, was estimated from a small-scale, pre-stained, three-point bend specimen. Fracture toughness values, evaluated by a CTOD test, were recently mandated for shipbuilding steel plates. The critical fracture toughness value is a very useful parameter to evaluate the safety of huge ship structures.