The effect of Zr addition on the melting temperature of the CoCrFeMnNi High Entropy Alloy (HEA), known as the “Cantor’s Alloy”, is investigated, together with its micro-structure, mechanical properties and thermomechanical recrystallization process. The base and Zr-modified alloys are obtained by vacuum induction melting of mechanically pre-alloyed powders. Raw materials are then cold rolled and annealed. recrystallization occurred during the heat treatment of the cold-rolled HEA. The alloys are characterized by X-ray diffraction, electron microscopy, thermal analyses, mechanical spectroscopy and indentation measures. The main advantages of Zr addition are: (1) a fast vacuum induction melting process; (2) the lower melting temperature, due to Zr eutectics formation with all the Cantor’s alloy elements; (3) the good chemical alloy homogeneity; and (4) the mechanical properties improvement of re-crystallized grains with a coherent structure. The crystallographic lattice of both alloys results in FCC. The Zr-modified HEA presents a higher recrystallization temperature and smaller grain size after recrystallization with respect to the Cantor’s alloy, with precipitation of a coherent second phase, which enhances the alloy hardness and strength.
The high entropy alloy (HEA) of equiatomic composition CrNiFeCoMn and with FCC crystal structure was additively manufactured in a selective laser melting (SLM) process starting from mechanically alloyed powders. The as-produced alloy shows fine nitride and σ phase precipitates, which are Cr-rich and stable up to about 900 K. The precipitates increase in number and dimensions after long-period annealing at 900–1300 K, with a change in the HEA mechanical properties. Higher aging temperatures in the furnace, above 1300 K, turn the alloy into a single FCC structure, with the disappearance of the nitride and σ phase precipitates inside the grains and at the grain boundaries, but still with the presence of a finer Cr-rich nitride precipitation phase. These results suggest that the as-produced HEA is a supersaturated solid solution at low and intermediate temperature with nitrides and σ nanostructures.
Several coating configurations on AISI 316 steel were obtained by a hot dipping process followed by isothermal interdiffusion. Six different kind of multilayered specimens were produced and characterized. These coatings, typically employed as bond coat in thermal barrier coating (TBC), can also be effective as vibration reduction elements at intermediate and high temperatures. This preliminary work was focused on the microstructural design and processing effects of the coatings. The damping of the produced specimens was measured up to 450 °C and compared with that of the steel substrate. The most performing coatings contain an Al-Si layer and exhibit a steep damping increase above 200 °C, reasonably due to dislocation movements by plastic straining of soft alloy layer and to the interface sliding between layers with different elastic moduli.
The effect of Zr addition on the melting temperature of the CoCrFeMnNi High Entropy Alloy (HEA), known as the “Cantor’s Alloy”, is investigated, together with its microstructure, mechan-ical properties and thermo-mechanical recrystallization process. The base and Zr-modified al-loys are obtained by vacuum induction melting of mechanically pre-alloyed powders followed by recrystallization. The alloys were characterized by X-ray diffraction, scanning and transmis-sion electron microscopy, thermal analyses, mechanical spectroscopy and indentation measures. The main advantages of Zr addition are: 1) a fast vacuum induction melting (VIM) process; 2) the lower melting temperature, due to Zr eutectics formation with all the Cantor’s alloy elements; 3) the good chemical alloy homogeneity; 4) the mechanical properties improvement of recrystallized grains with a coherent structure. The crystallographic lattice of both alloys resulted to be FCC. Results demonstrate that the Zr-modified HEA presents a higher recrystallization temperature and smaller grain size after recrystallization with respect to the Cantor’s alloy, with precipita-tion of a coherent second phase which enhance the alloy hardness and strength, while maintaining a good tensile ductility.
The high entropy alloy (HEA) of equiatomic composition CrNiFeCoMn and with FCC crystal structure was additively manufactured with a selective laser melting (SLM) process starting from mechanically alloyed powders. The as produced alloy shows finenitride and phase pre-cipitates, which are Cr-rich and stable up to about 900 K. The precipitates increase in number and dimensions after long-period annealing at 900-1300 K, with a change in the HEA mechanical properties. Higher aging temperatures in furnace, above 1300 K, turn the alloy in a single FCC structure, with disappearance of the nitrate and phase precipitates inside the grains and at the grain boundaries, but with still a presence of a finer Cr-rich nitride precipitation phase. These re-sults suggest that the as-produced HEA is a supersatured solid solution at low and intermediate temperature with nitrides and nanostructures.
The equiatomic high-entropy alloy of composition of CrNiCoFeMn with an FCC crystal structure was prepared by either induction melting or additive manufacturing with a selective laser melting (SLM) process, starting from mechanically alloyed powders. The as-produced samples of both kinds were cold worked, and in some cases re-crystallized. Unlike induction melting, there is a second phase, which is made of fine nitride and Cr-rich σ phase precipitates, in the as-produced SLM alloy. Young’s modulus and damping measurements, as a function of temperature in the 300–800 K range, were performed on the specimens that were cold-worked and/or re-crystallized. Young’s modulus values of (140 ± 10) GPa and (90 ± 10) GPa were measured from the resonance frequency of free-clamped bar-shaped samples at 300 K for the induction-melted and SLM samples, respectively. The room temperature values increased to (160 ± 10) GPa and (170 ± 10) GPa for the re-crystallized samples. The damping measurements showed two peaks, which were attributed to dislocation bending and grain-boundary sliding. The peaks were superposed on an increasing temperature background.