Atmospheric plasma-sprayed FeCrAl coatings possess heterogeneous lamellar structures whose characterization is important for interpreting friction and wear. This study compared four as-sprayed FeCrAl coatings produced at nominal powder feed rates of 25–40 g/min and a common stand-off distance of 150 mm. The objective was to compare their microstructural and surface characteristics with their room-temperature dry-sliding responses, particularly the correspondence between friction and wear rankings. The coatings were examined using SEM/EDS, X-ray diffraction, cross-sectional image analysis, surface profilometry, instrumented indentation, and ball-on-disk testing. Mean coating thicknesses ranged from 162 to 702 µm, while region-specific apparent porosity estimates ranged from 0.38 to 1.49%. The coatings exhibited heterogeneous lamellar microstructures and broadly similar diffraction patterns dominated by an α-Fe-type bcc matrix containing Cr, with additional reflections assigned to Fe3O4. The mean Ra values ranged from 22.83 ± 0.13 to 26.91 ± 0.36 µm (mean ± SD, n = 3), and individual indentations revealed substantial variation in local mechanical response. F3 exhibited the lowest measured specific wear rate of 1.051 × 10−4 mm3/(N·m) among the tested specimens. F4 showed the lowest approximate post-running-in friction coefficient of 0.77–0.80, whereas F1 exhibited the highest measured specific wear rate of 1.982 × 10−4 mm3/(N·m). Thus, the friction and wear rankings differed, and neither the measured roughness nor the region-specific apparent porosity alone accounted for the wear ranking. These findings characterize the tested specimens; one sliding test per coating and incomplete deposition records preclude establishing reproducibility or attributing the differences exclusively to powder feed rate.
In this study, we examined the influence of coating thickness on surface roughness, hardness, phase composition, and tribological behavior of arc-sprayed FeCrAl coatings deposited on steel substrates. We measured coating thickness, phase composition, and surface roughness using optical microscopy, X-ray diffraction (XRD), and profilometry, respectively. Results showed that surface roughness decreased with increasing coating thickness due to improved splat coalescence. However, Rockwell hardness remained nearly constant (at approximately 95 HRB), denoting a limited dependency on coating thickness. Using pin-on-disk tribometry, we found that the thickest coating showed the highest coefficient of friction (CoF, mean value of 0.864). This is because there is an in-creased tendency for the formation of hard oxide phases (Cr₂O₃ and Al₂O₃) in thicker coatings. These oxides increased friction by generating abrasive debris during sliding. The novelty of this work is that CoF is sensitive not only to surface morphology but also to thickness-dependent phase composition, whereas most previous studies found that CoF was primarily correlated with surface roughness only. Our research findings show that both microstructural and phase composition behavior during deposition are crucial for optimizing the friction and wear properties of FeCrAl coatings in high-temperature, steam-rich applications. Therefore, accurate control of oxidation behavior as a function of coating thickness can lead to more durable, reliable coatings in those environments.