In this study, the cause of failure of a low-carbon steel pipe meeting standard KS D 3562 (ASTM A135), in a district heating system was investigated. After 6 years of operation, the pipe failed prematurely due to pitting corrosion, which occurred both inside and outside of the pipe. Pitting corrosion occurred more prominently outside the pipe than inside, where water quality is controlled. The analysis indicated that the pipe failure occurred due to aluminum inclusions and the presence of a pearlite inhomogeneous phase fraction. Crevice corrosion occurred in the vicinity around the aluminum inclusions, causing localized corrosion. In the large pearlite fraction region, cementite in the pearlite acted as a cathode to promote dissolution of surrounding ferrite. Therefore, in the groundwater environment outside of the pipe, localized corrosion occurred due to crevice corrosion by aluminum inclusions, and localized corrosion was accelerated by the large fraction of pearlite around the aluminum inclusions, leading to pipe failure.
This study investigated the hydrogen embrittlement (HE) characteristics of advanced high-strength steels (AHSSs). Two different types of AHSSs with a tensile strength of 1.2 GPa were investigated. Slow strain rate tests (SSRTs) were performed under various applied potentials (Eapp) to identify the mechanism with the greatest effect on the embrittlement of the specimens. The SSRT results revealed that, as the Eapp increased, the elongation tended to increase, even when a potential exceeding the corrosion potential was applied. Both types of AHSSs exhibited embrittled fracture behavior that was dominated by HE. The fractured SSRT specimens were subjected to a thermal desorption spectroscopy analysis, revealing that diffusible hydrogen was trapped mainly at the grain boundaries and dislocations (i.e., reversible hydrogen-trapping sites). The micro-analysis results revealed that the poor HE resistance of the specimens was attributed to the more reversible hydrogen-trapping sites.
The automobile industry commonly uses cyclic corrosion tests (CCTs) to evaluate the durability of materials. However, the extended evaluation period required by CCTs can pose challenges in this fast-paced industry. To address this issue, a new approach that combines a CCT with an electrochemically accelerated corrosion test has been explored, to shorten the evaluation period. This method involves the formation of a corrosion product layer through a CCT, which leads to localized corrosion, followed by applying an electrochemically accelerated corrosion test using an agar gel electrolyte to preserve the corrosion product layer as much as possible. The results indicate that this approach can achieve comparable localized corrosion resistance, with similar localized corrosion area ratios and maximum localized corrosion depths to those obtained through a conventional CCT in half the time.
A new lifespan evaluation method, accelerated galvanic corrosion testing (AGCT), was developed for evaluating the lifespan of aluminum heat exchangers during the materials development stage. AGCT effectively accelerated corrosion by adjusting the polarization magnitude, which aligns with the polarization direction of sacrificial anode cathodic protection (SACP). Increasing the zinc content in the fin alloy (1.8 wt%, 2.2 wt%, 2.6 wt%, and 3.0 wt%) enhanced the SACP effect, with a 3.0 wt% Zn resulting in a 49% increase in the penetration lifespan of the heat exchanger. Galvanic simulation has confirmed that protection of the tube and filler is provided at zinc contents of 2.2 wt% or higher, but there is evidence of overprotection at 3.0 wt% Zn. Therefore, the optimal zinc content of fin was determined to be 2.6 wt%, which is expected to improve the heat exchanger penetration lifespan by up to 43%.
This study investigated the corrosion behavior of ADC12 and A365 aluminum alloys for automotive parts in the context of the growing use of aluminum parts in electric vehicles. Only ADC12 exhibited the formation of Al(OH)3 particle layer after corrosion, which was attributed to the microgalvanic effect influenced by the geometry characteristics of its microstructure. Results revealed that ADC12 was prone to forming Al(OH)3 particle layers due to the geometric effects of Si and θ-Al2Cu, which facilitates the isolation of α-Al. The distribution of band-shaped galvanic currents, concentrated in a small α-Al matrix region, was primarily governed by the geometry of Si, creating a preferred structure for α-Al isolation. Additionally, the geometry of θ-Al2Cu contributed to a significant increase in electrochemical kinetics, particularly at the tri-metallic coupled region, further enhancing the susceptibility of the isolation. As a result, the formation of the Al(OH)3 particle layer was attributed to the corrosion of isolated α-Al particles, generated through the synergistic effect of microgalvanic corrosion. Moreover, the corrosion attack progressed along the eutectic Si network, accompanied by θ-Al2Cu. Overall, the corrosion mechanism of ADC12 and A365 alloy was proposed.
This study investigates the impact of cathodic protection design on the corrosion resistance of heat exchangers (HE1, HE2). Two distinct heat exchanger assemblies underwent a 720-h cyclic corrosion test, revealing higher corrosion resistance in HE2 compared to HE1. The difference in cathodic protection design was observed at the fin-tube junction, where variations in the filler metal composition played a crucial role. Corrosion resistance was primarily influenced by the cathodic protection design at this junction rather than by the header-tube junction or the inherent corrosion susceptibility of the tube. Boundary element method simulations quantitatively confirmed that the tube’s corrosion resistance was supported by the current provided at the fin-tube junction, particularly across the fin-free zone. Optimization of the cathodic protection design was achieved by adjusting the Zn content in the filler metal at the fin-tube junction. These findings provide valuable insights for enhancing corrosion resistance in practical heat exchanger applications.