This paper presents the experimental results of self-healing efficiency of two different bacteria namely Bacillus sphaericus and Bacillus subtilis incorporated in with polypropylene fibre reinforced concrete. Concrete was prepared with an optimum amount of polypropylene fibre and cultured bacteria. The artificial cracks were formed in the concrete to perform this investigation. The cracked concrete was observed at constant intervals. The effectiveness of self-healing was evaluated by the mechanical test over the bacterial concrete with fibre (BCF). The results obtained from the mechanical study show that the BCF produced commendable results. The precipitation characteristic analysis was carried out by SEM and XRD diffractogram analysis was performed to confirm the precipitation in BCF. The analysis shows that there is a presence of sufficient self-healing compound in cracked concrete. The effectiveness of the developed BCF concrete in regaining strength shows a substantial increase in strength after self-healing therefore, the effectiveness of self-healing of BCF is admirable.
16 September 2017 in International Journal of Engineering & Technology
Cement consumption is increasing day by day due to the tremendous development in the infrastructure facilities. The production of one ton of cement emits approximately one ton of carbon dioxide to the atmosphere. In order to reduce the use of cement a new-generation concrete has been developed such as geopolymer concrete (GPC).Geopolymer Geopolymer is a new material which has the potential to replace ordinary Portland cement. It is an inorganic material synthesized by alkali activation of amorphous aluminosilicates at ambient or slightly increased temperatures having an amorphous to semi-crystalline polymeric structure. In this study, low calcium flyash from Tuticorin was used to produce geopolymer concrete. The geopolymer was synthesized with sodium silicate and sodium hydroxide solutions. The sodium hydroxide pellets was dissolved in the distilled water to make free from mixing water contaminants. The ratio of sodium silicate and sodium hydroxide ratio was kept as 2.5. The concentration of sodium hydroxide solution is 12 Molarity (12M). Other materials used are locally available coarse aggregate and fine sand in surface dry condition. A polycarboxlate HRWRA La Hypercrete S25was used. Cubes of size 100mm were cast for six mix proportions of 450kg/m3 flyash+0.35W/B, 500 kg/m3 flyash+0.35W/B, 550kg/m3 flyash+0.35W/B, 450kg/m3 flyash+.0.40 W/B, 500kg/m3 fly ash+0.40W/B and 550kg/m3 flyash+0.40W/B. The specimens after casting in moulds were kept in oven at 60°C for 6 hours and left to air dry at room temperature and tested at 7 and 28 days. The test results revealed the compressive strength of 30 Mpa was achieved. There was not much significant difference in strength development at 28 days between the mixes due to the increase of flyash content. The microstructural images at 28 days revealed that there was not much difference in the microstructure due to the variation in flyash content from 450 kg/m3 to 550 kg/m3.
This paper deals with the experimental investigation on the mechanical, thermal and moisture properties of Ground Granular Blast Furnace Slag (GGBS) based Geopolymer Pervious Concrete (GGPC) with different size of aggregates. The concentration of NaOH is maintained as 12 M throughout the study. Fine aggregate is completely eliminated in the mix proportion to maintain the pervious nature. Coarse aggregate size is varied in three sizes such as 6mm, 12mm, and 20mm to study the effect of aggregate on the properties of GGPC. The ratio between sodium silicate and sodium hydroxide is maintained as 2.5 throughout the study, and the liquid to solid ratio is maintained as 0.45. The results from the experiments revealed that the compressive strength is higher for the aggregate size 12 mm at the end of 28 days compared to other mixes. The Co-efficient of Permeability (k) is increased with respect to the increase in the aggregate size from 6 to 20 mm.
1 October 2019 in IOP Conference Series: Materials Science and Engineering
Due to the ample advantages and quite a lot of applications, 'Geopolymer concrete' is considered to be the alternative of conventional concrete. Moreover it is an eco-friendly and pollution controlled construction materials. The prime objective of this present study is to examine the effect of different activator ratio on the compressive strength of Ground Granulated Blast Furnace Slag(GGBS) based geopolymer concrete. The alkaline solution used in this study is sodium hydroxide (NaOH) and sodium silicate (Na2SiO3) in the ratio of 1:2 ½. Cube specimens of size 100 x 100 x100 mm are cast and cured at ambient temperature. This study results concluded that the activator ratio 0.30 performs well under compressibility studies.
1 February 2023 in Proceedings of the Institution of Civil Engineers - Engineering Sustainability
Alkali-activated binders are emerging sustainable binders in the construction sector due to their higher strength and superior resistance against aggressive environments than those of cement concrete. Steatite powder is obtained as a by-product of soapstone processing and disposed of as waste in large quantities. Studies on the reuse of steatite powder in alkali-activated concrete are few. Hence, the current research focuses on the influence of ultra-fine steatite powder on the mechanical as well as durability properties of slag- and fly-ash-based alkali-activated concrete. Six replacement levels (10, 20, 30, 40, 50 and 60%) of slag and fly ash with steatite powder were adopted and activated using a sodium-based activator. Heat curing and ambient curing were performed for fly ash–steatite concrete and slag–steatite concrete, respectively. From the test results, 30% steatite powder is the optimum for slag- and fly-ash-based alkali-activated concretes. Less water absorption and higher resistance against acid exposure are observed for steatite-based alkali-activated concrete specimens.