In situ graphene was grown on the surface of copper particles using highland barley powder, which is rich in sucrose and β-glucan, as a carbon source. The graphene content in the graphene-coated copper (Gr@Cu) composite powder was 4.98 wt.%. A characteristic angle of approximately 14° was observed between the graphene and copper crystal planes, indicating strong interfacial bonding. Raman spectroscopy revealed an ID/IG ratio of 0.96 for the graphene. Owing to the in situ growth of graphene, the mechanical properties of the copper matrix are effectively strengthened. At a graphene content of 0.7 wt.%, the graphene was uniformly dispersed within the copper matrix, resulting in optimized mechanical properties of the composite. This composite exhibited a conductivity of 70% IACS and a compressive yield strength of 175 MPa.