Ceramics have a history of use in total hip replacement (THR) including early use in hip resurfacing. Improvements in ceramics over the past two decades have resulted in the BIOLOX® delta material which has a higher fracture resistance, low wear and excellent biocompatibility compared to other orthopaedic biomaterials. Cobalt Chromium Molybdenum (CoCrMo) metal alloy continues to be used in hip resurfacing but is generally limited to use of larger sizes in active males due to a legacy of concerns with metal ion release from discontinued devices and large diameter modular head trunnions. A novel hip resurfacing device (ReCerf®, MatOrtho Ltd., UK) utilises BIOLOX® delta, removing CoCrMo metal from the prosthesis. ReCerf® is based on a clinically successful design from the same manufacturer (ADEPT®, MatOrtho Ltd., UK) and although BIOLOX® delta is a clinically proven material in THR, it requires significant testing to prove safety in the clinical environment. Increasing regulations particularly in Europe, has increased the time to market for new devices such as this and whilst the changes are being implemented to ensure the lowest risk for patients, they are also leaving patients unable to access new treatment routes. Ultimately, it is long term clinical outcomes that are required to determine whether the future of resurfacing is in using alternative materials such as ceramic and whether these compare favourably with the established, successful metal designs which have been in clinical use for over 20 years.
7 July 2020 in Proceedings of the Institution of Mechanical Engineers, Part H: Journal of Engineering in Medicine
A novel thin-walled direct-to-bone fixation ceramic cup was tested under critical impact loads simulating lateral fall and car crash scenarios. Three sizes of BIOLOX delta ceramic cups (total hip replacement cup with bearing diameter of 32 mm and two hip resurfacing cups with bearing diameters of 40 and 64mm) were implanted into reamed Sawbones blocks representing acetabulae. Three cups of each size were fully supported by the block and three were implanted with 15° of the cup’s outer diameter unsupported by the block. All testing was conducted with the corresponding bearing diameter heads lateralised by approximately 1 mm to represent worst case subluxed hips and all then subjected to test, replicating a lateral fall impact followed by a car crash impact. All cups passed lateral fall conditions without visible damage, although some movement of the cups was measured and damage to the blocks was observed. Five out of six of each cup size survived the car crash impacts with one fracture per size. In all cases, this was in the fully supported condition representing the highest cup inclination angle. The car crash impact force was equivalent to that reported to fracture the acetabulum and in all simulated cases, the Sawbones block showed signs of damage. Survival of five cups per size suggests the pelvis is much more likely to fracture before the cup. The ability of the cups to withstand these critical impact forces indicates they are unlikely to fracture in normal clinical use and should meet the more challenging demands of active patients likely to receive this device.
Hip resurfacing is a bone-conserving alternative to total hip replacement particularly suited to younger or more active patients with good bone stock. Historical issues with metal-on-metal hip resurfacing devices have led to investigations of new materials. In this study, the wear of a BIOLOX delta ceramic-on-ceramic hip resurfacing under a range of activities of daily function was investigated in an experimental simulation model. Under a standard walking gait, increased frequency, and stop–dwell–start conditions, the wear of the ceramic head and cup was low and at the limit of the sensitivity of the measurement technique used (<0.1 mm3/million cycles). Only when tested under a jogging-like protocol with higher loading (maximum 4.5 kN) coupled with higher frequency (1.25 Hz), under both continuous running and stop–dwell–start conditions, was wear measurable but still low, with a mean <0.15 mm3/million cycles. At the conclusion of the study, no wear scar was visible on any components and no changes in the surface roughness of the implants was measured. This short-term, pre-clinical study showed low wear of BIOLOX delta ceramic-on-ceramic hip resurfacings when evaluated under a range of activities of daily living and that this material combination has potential for the next generation of large-diameter hip bearings.
Morse-type tapers at the head–stem junction in total hip replacements (THRs) provide many benefits to permit a successful surgical outcome. However, with the introduction of modular tapered devices comes complications associated with fluid ingress and motion at the interface that can cause fretting corrosion, which has been implicated in clinical failure. Increased surface roughness amplitude (Ra) and angular mismatch to ensure taper contact closer to the equator of the femoral head are design features introduced for use with ceramic heads but have been adopted by metal head couples. While increased surface roughness amplitude has been found to contribute to fretting corrosion, there is a distinct lack of systematic studies investigating the interactions between angular mismatch and Ra. This study measured the fretting corrosion and motion response of clinically representative samples, in part reference to ASTM F1875, when subjected to uniaxial incremental dynamic loading. The fretting corrosion response was measured in situ with an integrated three electrode electrochemical cell. Motion at the head–neck interface was measured with a bespoke motion measurement solution based on eddy-current principles which uses four sensors to allow motion to be fully characterised in three dimensions. Key findings from this study included a 5–10-fold increase in current measured in the increased roughness amplitude samples, suggesting an increased susceptibility to fretting corrosion without a corresponding increase in motion. The distal samples engaged around the opening of the taper interface and presented the lowest current measurements but most off-axis subsidence. Findings from this study indicate that optimisation of the taper interfaces in THR, in terms of fretting corrosion and motion, can be made and can be assessed using short-term preclinical tests.