This study investigates a silica-gel-supported cobalt catalyst for synthesizing long-chain hydrocarbons (C19+) from CO and H2. The process conditions were varied within the following ranges: pressure, 1.5–3.5 MPa; gas hourly space velocity (GHSV), 300–830 h–1; H2/CO ratio, 2.0–2.3; and temperature, 187–213°C. Catalytic testing revealed a correlation between the catalyst deactivation rate and the content of C19+ hydrocarbons in the products. When the C19+ content increased from approximately 40 to 55 wt %, the deactivation rate increased more than tenfold. Under optimized conditions (H2/CO = 2.3, P = 2.0 MPa, T = 193°C), the C19+ content reached ~46–50 wt %, and the deactivation rate was minimized. A long-term stability test over 500 h was used to project a catalyst cycle length, which was found to be at least 4000 h. The study results provide a foundation for optimizing Fischer–Tropsch process conditions to maximize catalyst lifetime and selectivity toward heavy hydrocarbons, supporting the recommendation of the proposed catalyst for industrial implementation.
Thermal pyrolysis of polyethylene (PE) under pressure and hydroisomerization over Pt/SAPO-11 are known separately; this work examines their integration. PE was pyrolyzed at 400–550 °C and constant pressures of 0.1–2.0 MPa, and the 140–280 °C fraction (pyrolysis kerosene) was hydroisomerized over 0.5 wt% Pt/SAPO-11. The yield of the 140–280 °C fraction decreases with temperature and increases with pressure, reaching 45.3 wt% at 400 °C and 1.0 MPa (27.4 wt% at 0.1 MPa); a control run under these conditions gave a directly measured gas yield of 13.2 wt% and a mass balance closure of 99.3%. The pyrolysis kerosene contains 47.6 wt% alkenes and 20.0 wt% cycloalkanes. Hydroisomerization at 6 MPa and a liquid hourly space velocity of 3 h−1 gives 91.1–93.4 wt% of the kerosene fraction (>140 °C) at 290–300 °C, with near-complete alkene hydrogenation; at 330 °C, the freezing point falls below −90 °C (pyrolysis kerosene: −13 °C), but hydrocracking reduces the yield to 72.4 wt%. The kerosene fraction obtained at the selected temperature of 300 °C (57.2% isoalkanes, 25.1% cycloalkanes, 0.1% aromatics) meets all measured GOST 10227-86 requirements for Russian RT jet fuel except density. The overall kerosene yield is 41.3 wt% of PE (40.0–40.4 wt% within the 140–280 °C boundaries). A preliminary estimate shows that the heat and hydrogen demand of the process corresponds to 68–97% of the energy of the pyrolysis gases.
This study proposes a method for selectively producing diesel-range hydrocarbons by combining Fischer–Tropsch synthesis (FTS) over a zeolite-supported catalyst with the oligomerization of C5–C10 alkenes over an H-Beta zeolite. FTS was carried out under gas recirculation conditions (H2/CO = 1.85, 2.0 MPa). At a recirculation ratio of 16, the diesel content in the product increased to 54.6 wt %, compared to 38.7 wt % under flow-through conditions. Finally, by oligomerizing the alkene-enriched gasoline fraction from the FTS over H-Beta-18, the overall diesel fuel content was enhanced to 69%.
This study investigates the effect of a cobalt-based component (selected from Co/SiO2, Co/C, and Co/ZrO2) on the physicochemical properties and catalytic performance of zeolite-containing composite catalysts for Fischer–Tropsch (FT) synthesis. The choice of catalyst support governs activity, selectivity toward liquid hydrocarbons, and the group composition of target products. Catalysts supported on SiO2 and ZrO2 showed similar CO conversion (~86%) and space-time yields (STY) of C5+ hydrocarbons (130–134 kg m–3 h–1). In contrast, the carbon-supported sample exhibited slightly lower CO conversion (71.7%) but superior C5+ selectivity (73.1%). Product distribution strongly depends on the support type: the ZrO2-supported catalyst gave the highest content of branched hydrocarbons (iso/n = 1.77); the SiO2-supported sample maximized olefin yield, indicative of low hydrogenating activity; and the carbon-supported sample excelled in high-molecular-weight (C19+) hydrocarbons (9.0 wt %). These results demonstrate that the FT product distribution can be tailored by an appropriate choice of the cobalt-based component.