A series of bifunctional cobalt composite catalysts supported on mixed zeolites were synthesized to enhance the selectivity towards liquid fuels rich in branched hydrocarbons. Given that the catalysts were prepared with an alumina binder and that the mixed zeolites consisted of two molecular sieves, the finished samples were generally formulated as Co–Al2O3/SiO2 + [ZSM-5 + (ZSM-23, Beta, SAPO-11)] + Al2O3. The catalysts were tested in Fischer–Tropsch synthesis at 240°C, 2.0 MPa, an H2/CO ratio of 2 : 1, and a syngas hourly space velocity (GHSV) of 1000 h–1. The catalyst supported on ZSM-5+Beta exhibited the highest selectivity towards C5–C10 hydrocarbons. The ZSM-5+ZSM-23-supported catalyst turned out to be the most selective towards branched hydrocarbons, which, in turn, favored the production of a diesel fraction with optimal low-temperature properties.
The effect of sodium and the method of its introduction on the physicochemical and catalytic properties of hybrid cobalt–zeolite catalysts in Fischer–Tropsch synthesis (FTS) was studied. Hybrid catalysts containing Co–Al2O3/SiO2 and ZSM-5 zeolite were prepared by mixing the components followed by extrusion. XRD, H2-TPR, NH3-TPD, and IR spectroscopy of adsorbed pyridine showed that the location of sodium determines its effect on catalyst structure and activity. The introduction of sodium into the Co–Al2O3/SiO2 catalyst was shown to increase the Co0 particle size from 9.0 to 14.0 nm and enhance the activity: CO conversion increases from 76.4 to 85.3%, while the C5+ productivity increases to 114.5 kg/(mcat3 h). In contrast, the introduction of sodium into the zeolite decreases the total acidity from 640 to 589 μmol/g and results in a substantial decrease in activity, with CO conversion decreasing from 85.6 to 66.2%, C5+ productivity decreasing by 35%, and the fractional composition shifting toward a higher proportion of high-molecular-weight C19+ hydrocarbons, from 8.3 to 15.6%. The residual sodium content in the zeolite was found to be a critical parameter determining the efficiency of the hybrid catalyst.
Thermal pyrolysis of polyethylene (PE) under pressure and hydroisomerization over Pt/SAPO-11 are known separately; this work examines their integration. PE was pyrolyzed at 400–550 °C and constant pressures of 0.1–2.0 MPa, and the 140–280 °C fraction (pyrolysis kerosene) was hydroisomerized over 0.5 wt% Pt/SAPO-11. The yield of the 140–280 °C fraction decreases with temperature and increases with pressure, reaching 45.3 wt% at 400 °C and 1.0 MPa (27.4 wt% at 0.1 MPa); a control run under these conditions gave a directly measured gas yield of 13.2 wt% and a mass balance closure of 99.3%. The pyrolysis kerosene contains 47.6 wt% alkenes and 20.0 wt% cycloalkanes. Hydroisomerization at 6 MPa and a liquid hourly space velocity of 3 h−1 gives 91.1–93.4 wt% of the kerosene fraction (>140 °C) at 290–300 °C, with near-complete alkene hydrogenation; at 330 °C, the freezing point falls below −90 °C (pyrolysis kerosene: −13 °C), but hydrocracking reduces the yield to 72.4 wt%. The kerosene fraction obtained at the selected temperature of 300 °C (57.2% isoalkanes, 25.1% cycloalkanes, 0.1% aromatics) meets all measured GOST 10227-86 requirements for Russian RT jet fuel except density. The overall kerosene yield is 41.3 wt% of PE (40.0–40.4 wt% within the 140–280 °C boundaries). A preliminary estimate shows that the heat and hydrogen demand of the process corresponds to 68–97% of the energy of the pyrolysis gases.