Optically detected magnetic resonance has been observed from GaN. Two magnetic resonances have been detected on the 2.2 eV-deep photoluminescence band. The first resonance is sharp [full width at half-maximum (FWHM) ∼2.2 mT] with g∥=1.9515±0.0002 and g⊥=1.9485±0.0002 and is assigned to conduction electrons, in agreement with recent electron paramagnetic resonance (EPR) studies of similar samples. The second feature, which has not been seen by EPR, is much broader (FWHM∼13 mT) with g∥=1.989±0.001 and g⊥=1.992±0.001. These parameters indicate a deep state. A tentative assignment is made to a deep state associated with the N vacancy.
Activation of implanted donors into a highly-resistive, nitrogen-doped homoepitaxial β-Ga2O3 has been investigated. Nitrogen acceptors with the concentration of ∼1017 cm−3 were incorporated during epitaxial growth yielding low-doped (net donor concentration <1014 cm−3) films subsequently implanted with Si, Ge, and Sn. Upon Ohmic contact formation to the implanted regions, sheet resistance values of 314, 926, and 1676 Ω/sq were measured at room temperature for the Si-, Ge-, and Sn-implanted samples, respectively. Room temperature Hall measurements resulted in sheet carrier concentrations and Hall mobilities of 2.13 × 1014 /93, 8.58 × 1013/78, and 5.87 × 1013/63 cm2/(V s), respectively, for these three donor species. Secondary ion mass spectroscopy showed a volumetric dopant concentration of approximately 2 × 1019 cm−3 for the three species, resulting in carrier activation efficiencies of 64.7%, 40.3%, and 28.2% for Si, Ge, and Sn, respectively. Temperature-dependent Hall effect measurements ranging from 15 to 300 K showed a nearly constant carrier concentration in the Si-implanted sample, suggesting the formation of an impurity band indicative of degenerate doping. With a bulk carrier concentration of 1.3 × 1019 cm−3 for the Si implanted sample, a room temperature mobility of 93 cm2/(V s) is among the highest reported in Ga2O3 with a similar carrier concentration. The unimplanted Ga2O3:N regions remained highly resistive after the surrounding areas received implant and activation anneal. These results open the pathway for fabricating Ga2O3 devices through the selective n-type doping in highly resistive epitaxial Ga2O3.
Electrical, optical, and structural properties of Si-doped GaN films grown on multiple AlN interlayers (IL) sandwiched between high-temperature (HT) GaN are presented. We show that as the number of AlN IL/HT GaN layers increases, the electron mobility increases in the top Si-doped GaN layer, showing a near doubling from 440 to 725 cm2 V−1 s−1. Cross-sectional transmission electron microscopy images reveal a significant reduction in the screw dislocation density for GaN films grown on the AlN IL/HT GaN layers. The symmetric and off-axis x-ray linewidths increase as the number of AlN IL/HT GaN layers increase, indicating a greater relative misalignment of the adjacent HT GaN layers. Photoluminescence spectra of undoped and Si-doped GaN films on the multiple AlN IL/HT GaN layers have small yellow-band intensity. Analysis based on a single-donor/single-acceptor model for the electrical conduction suggests that the improved electron mobility is the result of a reduced acceptor concentration in the top GaN film and that this acceptor may possibly be associated with threading screw dislocations in GaN.
The real dielectric constant for chemical vapor deposition 3C‐SiC grown on silicon (Si) has been determined at 300 K and at 5 K from an analytic fit to interference fringes in transmission over the spectral range from the near infrared to the submillimeter region. This technique is capable of high accuracy being limited typically by the sample thickness and accuracy with which the thickness is measured. The resulting real dielectric constant is lower than the values usually attributed to this material. We find: at 300 K ε 0=9.52 and ε ∞=6.38; at 5 K ε0=9.28 and ε ∞=6.22. In all cases the estimated error is ±0.8%. The observed ratio ε0 /ε∞ agrees with the Lyddane–Sachs–Teller relation to 0.1% at 300 K and 0.2% at 5 K.