Experimental dental resin composites incorporating copper-doped mesoporous bioactive glass nanospheres (Cu-MBGN) were designed to impart antibacterial and remineralizing properties. The study evaluated the influence of Cu-MBGN on the mechanical properties and photopolymerization of resin composites. Cu-MBGN were synthesized using a microemulsion-assisted sol–gel method. Increasing amounts of Cu-MBGN (0, 1, 5, and 10 wt %) were added to the organic polymer matrix with inert glass micro- and nanofillers while maintaining a constant resin/filler ratio. Six tests were performed: X-ray diffraction, scanning electron microscopy, flexural strength (FS), flexural modulus (FM), Vickers microhardness (MH), and degree of conversion (DC). FS and MH of Cu-MBGN composites with silica fillers showed no deterioration with aging, with statistically similar results at 1 and 28 days. FM was not influenced by the addition of Cu-MBGN but was reduced for all tested materials after 28 days. The specimens with 1 and 5% Cu-MBGN had the highest FS, FM, MH, and DC values at 28 days, while controls with 45S5 bioactive glass had the lowest FM, FS, and MH. DC was high for all materials (83.7–93.0%). Cu-MBGN composites with silica have a potential for clinical implementation due to high DC and good mechanical properties with adequate resistance to aging.
The objective of this study was to compare the polymerization kinetics of bulk-fill resin composites cured with a LED-curing device and a diode laser (449 nm). Three bulk-fill composites were light-cured with constant radiation exposure at 10 J/cm2 by varying radiant exitance and curing time. The following three light-curing protocols were used: (I) 3300 mW/cm2 for 3 s; (II) 2000 mW/cm2 for 5 s; and (III) 1000 mW/cm2 for 10 s. The degree of conversion (DC) was monitored in real time at a data acquisition rate of 2 spectra/s over a 5-min period and again after seven days using Fourier transform infrared spectroscopy. DC amounted to 30.9–61.7% at 4-mm depth after 5 min. DC values of two sculptable composites were significantly higher with the laser, regardless of the curing protocol used, but not for the flowable composite. The maximum polymerization rate (2.0–22.1%/s) was less affected by the type of curing device for one of the composites, while the other two composites achieved significantly higher values when cured with the laser. Laser curing generally increased the DC and the maximum polymerization rate while it shortened the onset of the maximum reaction rate. New handheld laser devices with adjustable power have the potential to be used as a photopolymerization light source for new generations of bulk-fill composites.
We embedded copper-doped mesoporous bioactive glass nanospheres (Cu-MBGN) with antibacterial and ion-releasing properties into experimental dental composites and investigated the effect of Cu-MBGN on the polymerisation properties. We prepared seven composites with a BisGMA/TEGDMA (60/40) matrix and 65 wt.% total filler content, added Cu-MBGN or a combination of Cu-MBGN and silanised silica to the silanised barium glass base, and examined nine parameters: light transmittance, degree of conversion (DC), maximum polymerisation rate (Rmax), time to reach Rmax, linear shrinkage, shrinkage stress (PSS), maximum PSS rate, time to reach maximum PSS rate, and depth of cure. Cu-MBGN without silica accelerated polymerisation, reduced light transmission, and had the highest DC (58.8 ± 0.9%) and Rmax (9.8 ± 0.2%/s), but lower shrinkage (3 ± 0.05%) and similar PSS (0.89 ± 0.07 MPa) versus the inert reference (0.83 ± 0.13 MPa). Combined Cu-MBGN and silica slowed the Rmax and achieved a similar DC but resulted in higher shrinkage. However, using a combined 5 wt.% Cu-MBGN and silica, the PSS resembled that of the inert reference. The synergistic action of 5 wt.% Cu-MBGN and silanised silica in combination with silanised barium glass resulted in a material with the highest likelihood for dental applications in future.
This study aimed to evaluate the micro-mechanical and macro-mechanical properties of self-cured and light-cured alkasite and to investigate how accelerated degradation in acidic, alkaline, and ethanol solutions affects the macro-mechanical properties of self-cured and light-cured alkasite. The specimens of the alkasite material (Cention Forte, Ivoclar Vivadent) were prepared according to the following three curing modes: (1) light-cured immediately, (2) light-cured after a 5-min delay, and (3) self-cured. Microhardness was tested before and after immersion in absolute ethanol to indirectly determine crosslink density, while flexural strength and flexural modulus were measured using a three-point bending test after accelerated aging in the following solutions: (1) lactic acid solution (pH = 4.0), (2) NaOH solution (pH = 13.0), (3) phosphate-buffered saline solution (pH = 7.4), and (4) 75% ethanol solution. The data were statistically analyzed using a two-way ANOVA and Tukey post hoc test. The results showed that the microhardness, flexural strength, and flexural modulus were significantly lower in self-cured specimens compared to light-cured specimens. A 5-min delay between the extrusion of the material from the capsule and light curing had no significant effect on any of the measured properties. A significant effect of the accelerated aging solutions on macro-mechanical properties was observed, with ethanol and alkaline solutions having a particularly detrimental effect. In conclusion, light curing was preferable to self-curing, as it resulted in significantly better micro- and macro-mechanical properties, while a 5-min delay between mixing the capsule and light curing had no negative effects.
This study investigated real-time polymerisation kinetics and mechanical properties under accelerated ageing of novel universal bulk-fill composites incorporating reversible addition–fragmentation chain transfer (RAFT) agent ß-allyl sulfone, designed for anterior and posterior applications. Five bulk-fill composites were tested: Tetric Plus Fill and Tetric Plus Flow (new universal composites); their predecessors, Tetric PowerFill and Tetric PowerFlow (Ivoclar); and RAFT-free Ecosite Bulk Fill (DMG). Specimens were polymerised for 3 s (~3000 mW/cm2), 10 s (~1200 mW/cm2), or 20 s (~1200 mW/cm2). Degree of conversion (DC) was monitored during and after curing, with mechanical testing after 24 h and after thermal cycling. DC and maximum polymerisation rate at 4 mm depth were significantly lower than at 0.1 mm for all materials and curing times. Three-second curing accelerated the polymerisation rate at both depths. Except for Ecosite cured for 3 or 10 s as RAFT-free material, DC ratios at 4 mm exceeded 80% of surface values. Tetric Plus Fill and Ecosite exhibited the highest flexural strength after 24 h, while PowerFill and Ecosite showed the highest flexural modulus at 24 h and after thermal cycling. Rapid curing did not compromise mechanical properties after 24 h, except for PowerFlow, the composite with the lowest filler vol%, but negatively affected both flowable composites after ageing. Thermal cycling reduced flexural strength in most tested conditions, but all materials and curing conditions more than satisfied the ISO 4049 requirements. The new simplified universal composite Plus Fill has a higher DC and improved polymerisation kinetics compared to its predecessor, PowerFill. Rapid curing is not recommended for the material without RAFT agents.