This article presents the results of an investigation of acoustic and thermophysical properties of insulation panels made from recycled technical textiles originating from the automotive industry. Measurements were performed on the samples of insulation panels (Senizol AT XX2 TL60), which were modified with liquid flame retardants (ISONEM® ANTI-FIRE SOLUTION, ECOGARD® B45, HR Prof). Another method of treatment was carried out by surface application of non-flammable facing (woven carbon fibre, nonwoven carbon fibre). Retardants were applied to the samples by surface spraying and soaking. The results showed a high ability of material to absorb sound in the frequency range 350 Hz–2 kHz. The sound absorption coefficient ranged from 0.82 to 0.9 in the frequency range 500 Hz–2 kHz. The noise reduction coefficient is 0.75. After material modification with the flame retardants, there was no significant change of sound absorption. The thermal conductivity coefficient of material before modification was 0.038 W⋅m−1⋅K−1. After application of the flame retardants, the thermal conductivity coefficient increased depending on type and method of retardant application in the range of 2.6–105.3%. The smallest change was detected after modification of material with ECOGARD® B45.
The influence of two commercial fire-retardant formulations, HR Prof and Krovsan, and their mixtures on the thermal behavior and fire resistance of spruce wood was evaluated by simultaneous thermal analysis STA (namely TG/DTG/DSC) and radiant-heat exposure. The untreated wood exhibited the typical three-stage degradation of lignocellulosic material with a maximum mass-loss rate near 265 °C. All treated specimens showed delayed decomposition, reduced oxidation rate, and markedly higher residual mass at 700 °C. A strong correlation was found between thermogravimetric residue and the mass retained after radiant-heat testing, confirming that improved performance resulted from condensed-phase stabilization. Phosphorus–nitrogen components of HR Prof promoted early dehydration and intumescence, while boron–copper species in Krovsan reinforced the carbonized layer and limited oxidation at elevated temperature. The balanced mixture (50 HR – 50 KR) provided the most effective protection, combining early char formation with long-term stability. The synergistic action of HR Prof and Krovsan thus offers an efficient and environmentally acceptable strategy for enhancing the fire safety of spruce wood.
In this study, we evaluate a phosphorus-based fire retardant (HR Prof) on Norway spruce using Simultaneous Thermal Analysis (STA: TG/DTG/DSC), Gas Chromatography–Mass Spectrometry (GC–MS), and bench-scale mass-loss measurements. Relative to the untreated reference, HR Prof re-routes decomposition toward earlier dehydration and transient char, simplifies the evolved gas mixture in the 150–250 °C range, and reduces burning intensity during 600 s of radiant exposure. Across 150/200/250 °C, identified components fell from 20/24/51 (reference) to 5/9/9 (HR Prof); no phosphorus-containing volatiles were detected in this window. Mass-loss tests showed a lower average burning rate (0.107 vs. 0.156%·s−1) and a smaller cumulative loss at 600 s (64.2 ± 9.5% vs. 93.7 ± 2.1%; one-way ANOVA, p < 0.05 for percentage loss). STA was conducted in air; the transient char formed at an intermediate temperature is oxidized near ~600 °C, explaining the low final residue despite earlier charring. A count-based Poisson model corroborated the significant reduction in volatile component richness for HR Prof (p < 0.001). The cross-method correspondences—earlier condensed-phase dehydration/char → leaner volatile pool → lower and flatter burning-rate profiles—support a condensed-phase-dominated protection mechanism within the conditions studied.
The fire response of cross-laminated timber (CLT) sandwich wall assemblies depends on interactions among the structural core, lining, cavities and secondary timber members. This study examines the thermal roles of these layers under medium-scale radiant exposure. The thermogravimetric mass change, mass-loss rate and heat-flow response were obtained for CLT, Fermacell® gypsum–fiber board and timber stud specimens by simultaneous thermal analysis. One complete, artifact-free record per material group was selected for mechanistic comparison; the data were not used to characterize material variability statistically. The degradation intervals were compared qualitatively with temperatures, visual observations and post-test damage recorded during a 90 min exposure of the wall assembly at 20 kW/m2. Fermacell® retained 77.8% of its initial mass; CLT and stud specimens retained 22.5% and 20.8%, respectively. The largest mass loss of both wood-based materials occurred at 280–430 °C, with mass-loss-rate peaks at 372.1 °C for the CLT and 359.4 °C for the stud. The lining initially delayed heat transfer. After board cracking, cavity heating was followed by the degradation and glowing of the timber stud. Layer-specific thermal analysis supports the mechanistic interpretation of the tested assembly, but it neither predicts event timing nor replaces standardized fire resistance testing or classification.